[en] The alloy composition is 10.2 Mo, 5.8 Zr, 4.7 Sn, 0.03 Fe, 0.014 N, 0.02 C, 0.13 O, bal. Ti. The fracture toughness increases with the solution treatment, but this effect lessens with decreasing test temperature. Solution treating above the beta transus resulted in a fracture toughness insensitive to test temperatures above 2730K; below, the toughness decreased almost linearly to 770K. Sub-transus treated alloy exhibited a linear toughness decrease over the entire temperature range. SEM observations are reported